Resources

In a materials characterization laboratory, undergraduate engineering students perform a tensile test on an annealed 1018 mild steel specimen using an MTS hydraulic universal testing system equipped with a calibrated 25.00-mm25.00\text{-mm} axial knife-edge extensometer. The specimen has a measured initial circular gauge diameter of d0=6.25 mmd_0 = 6.25\text{ mm}. The lab data acquisition system logs the following discrete load-deformation points within the initial linear regime:

  • Point 1: F1=3.20 kNF_1 = 3.20\text{ kN}, extensometer gauge reading L1=25.0065 mmL_1 = 25.0065\text{ mm}
  • Point 2: F2=7.80 kNF_2 = 7.80\text{ kN}, extensometer gauge reading L2=25.0159 mmL_2 = 25.0159\text{ mm}

Beyond this linear portion, the specimen exhibits a sharp upper yield drop at Fyield=11.20 kNF_{\text{yield}} = 11.20\text{ kN}. Based strictly on this laboratory dataset: (a) calculate the Young's modulus EE of the steel using the linear regression slope Δσ/Δε\Delta \sigma / \Delta \varepsilon between Points 1 and 2, and (b) determine the engineering yield strength σy\sigma_y of the specimen in megapascals (MPa\text{MPa}).

Answer and steps

Final answer

(a) E=2.00×1011 Pa=200 GPaE = 2.00 \times 10^{11}\text{ Pa} = 200\text{ GPa}; (b) σy=365 MPa\sigma_y = 365\text{ MPa}

Steps

01

Calculate the Original Cross-Sectional Area

The initial cross-sectional area A0A_0 of the circular gauge section is:

A0=π4d02A_0 = \frac{\pi}{4} d_0^2

Substituting the initial diameter d0=6.25 mm=6.25×10−3 md_0 = 6.25\text{ mm} = 6.25 \times 10^{-3}\text{ m}:

A0=π4(6.25×10−3 m)2≈3.068×10−5 m2=30.68 mm2A_0 = \frac{\pi}{4} (6.25 \times 10^{-3}\text{ m})^2 \approx 3.068 \times 10^{-5}\text{ m}^2 = 30.68\text{ mm}^2


02

Determine the Slope and Young's Modulus (EE)

Hooke's law in the linear elastic regime defines Young's modulus as the ratio of tensile stress change Δσ\Delta \sigma to tensile strain change Δε\Delta \varepsilon:

E=ΔσΔε=ΔF/A0ΔL/L0=ΔF⋅L0A0⋅ΔLE = \frac{\Delta \sigma}{\Delta \varepsilon} = \frac{\Delta F / A_0}{\Delta L / L_0} = \frac{\Delta F \cdot L_0}{A_0 \cdot \Delta L}

Using the data points recorded in the linear regime:

  • Change in applied tensile force: ΔF=F2−F1=7.80 kN−3.20 kN=4.60 kN=4600 N\Delta F = F_2 - F_1 = 7.80\text{ kN} - 3.20\text{ kN} = 4.60\text{ kN} = 4600\text{ N}
  • Change in gauge elongation: ΔL=L2−L1=25.0159 mm−25.0065 mm=0.0094 mm=9.4×10−6 m\Delta L = L_2 - L_1 = 25.0159\text{ mm} - 25.0065\text{ mm} = 0.0094\text{ mm} = 9.4 \times 10^{-6}\text{ m}
  • Gauge length: L0=25.00 mm=0.025 mL_0 = 25.00\text{ mm} = 0.025\text{ m}

Substitute these values into the modulus formula:

Δσ=4600 N3.068×10−5 m2≈1.499×108 Pa=149.9 MPa\Delta \sigma = \frac{4600\text{ N}}{3.068 \times 10^{-5}\text{ m}^2} \approx 1.499 \times 10^8\text{ Pa} = 149.9\text{ MPa}

Δε=ΔLL0=0.0094 mm25.00 mm=3.76×10−4\Delta \varepsilon = \frac{\Delta L}{L_0} = \frac{0.0094\text{ mm}}{25.00\text{ mm}} = 3.76 \times 10^{-4}

E=1.499×108 Pa3.76×10−4≈2.00×1011 Pa=200 GPaE = \frac{1.499 \times 10^8\text{ Pa}}{3.76 \times 10^{-4}} \approx 2.00 \times 10^{11}\text{ Pa} = 200\text{ GPa}


03

Calculate the Engineering Yield Strength (σy\sigma_y)

The engineering yield strength is defined as the applied load at the onset of yielding divided by the original cross-sectional area:

σy=FyieldA0\sigma_y = \frac{F_{\text{yield}}}{A_0}

Given Fyield=11.20 kN=11200 NF_{\text{yield}} = 11.20\text{ kN} = 11200\text{ N}:

σy=11200 N3.068×10−5 m2≈3.65×108 Pa=365 MPa\sigma_y = \frac{11200\text{ N}}{3.068 \times 10^{-5}\text{ m}^2} \approx 3.65 \times 10^8\text{ Pa} = 365\text{ MPa}

Pitfall to avoid: Always use the original gauge length L0=25.00 mmL_0 = 25.00\text{ mm} and original cross-sectional area A0A_0 when computing engineering strain, stress, and yield strength, rather than instantaneous dimensions.

Typical errors

OverviewACEpath Teacher's Diagnosis

01 The student confuses the diameter with the radius when calculating the cross-sectional area, using π d₀² instead of π d₀² / 4, which underestimates the stress, Young's modulus, and yield strength by a factor of 4.

Sample Student Work

Reviewed by ACEpath Teacher
Step-by-Step Review
Walk Through It with Your Teacher
Incorrect
  1. Step 1

    A0=πd02=π(6.25 mm)2=122.72 mm2A_0 = \pi d_0^2 = \pi (6.25\text{ mm})^2 = 122.72\text{ mm}^2

    Correct

    A0=π4d02=π4(6.25 mm)2≈30.68 mm2A_0 = \frac{\pi}{4} d_0^2 = \frac{\pi}{4} (6.25\text{ mm})^2 \approx 30.68\text{ mm}^2

    You calculated the area using d0d_0 directly in πd2\pi d^2 rather than π4d2\frac{\pi}{4}d^2 or π(d2)2\pi \left(\frac{d}{2}\right)^2. A circle's area is πr2\pi r^2, which equals π4d2\frac{\pi}{4}d^2.

  2. Step 2

    ΔF=7.80 kN−3.20 kN=4.60 kN=4600 N  ⟹  Δσ=4600 N/122.72 mm2=37.48 MPa\Delta F = 7.80\text{ kN} - 3.20\text{ kN} = 4.60\text{ kN} = 4600\text{ N} \implies \Delta \sigma = 4600\text{ N} / 122.72\text{ mm}^2 = 37.48\text{ MPa}

    Correct

    Δσ=ΔFA0=4600 N30.68 mm2≈149.9 MPa\Delta \sigma = \frac{\Delta F}{A_0} = \frac{4600\text{ N}}{30.68\text{ mm}^2} \approx 149.9\text{ MPa}

    Your force difference ΔF=4600 N\Delta F = 4600\text{ N} is correct, but your stress calculation used the incorrect area A0A_0 from Step 1.

  3. Step 3

    ΔL=25.0159 mm−25.0065 mm=0.0094 mm  ⟹  Δε=0.0094 mm25.00 mm=0.000376\Delta L = 25.0159\text{ mm} - 25.0065\text{ mm} = 0.0094\text{ mm} \implies \Delta \varepsilon = \frac{0.0094\text{ mm}}{25.00\text{ mm}} = 0.000376

  4. Step 4

    E=ΔσΔε=37.48 MPa0.000376=99681 MPa≈9.97×104 MPaE = \frac{\Delta \sigma}{\Delta \varepsilon} = \frac{37.48\text{ MPa}}{0.000376} = 99681\text{ MPa} \approx 9.97 \times 10^4\text{ MPa}

    Correct

    E=ΔσΔε=149.9 MPa3.76×10−4≈2.00×105 MPa=200 GPaE = \frac{\Delta \sigma}{\Delta \varepsilon} = \frac{149.9\text{ MPa}}{3.76 \times 10^{-4}} \approx 2.00 \times 10^5\text{ MPa} = 200\text{ GPa}

    Your definition of Young's modulus as the ratio Δσ/Δε\Delta \sigma / \Delta \varepsilon is correct, but the numerical result is reduced by a factor of 4 due to the area error.

  5. Step 5

    σy=FyieldA0=11200 N122.72 mm2=91.27 MPa≈91.3 MPa\sigma_y = \frac{F_{\text{yield}}}{A_0} = \frac{11200\text{ N}}{122.72\text{ mm}^2} = 91.27\text{ MPa} \approx 91.3\text{ MPa}

    Correct

    σy=FyieldA0=11200 N30.68 mm2≈365 MPa\sigma_y = \frac{F_{\text{yield}}}{A_0} = \frac{11200\text{ N}}{30.68\text{ mm}^2} \approx 365\text{ MPa}

    You applied the correct engineering yield strength relation, but substituting the incorrect area yielded 91.3 MPa91.3\text{ MPa} instead of 365 MPa365\text{ MPa}.

WHAT YOU DID WELL
Compliments from Your Teacher

You calculated both increments ΔF\Delta F and ΔL\Delta L accurately from the laboratory dataset.

You correctly used the original gauge length L0=25.00 mmL_0 = 25.00\text{ mm} to compute engineering strain.

You applied the correct definitions for both Young's modulus and engineering yield strength.

THE ERROR
Where Your ACEpath Teacher Spotted the Mistake
Area Formula Error

You wrote πd02\pi d_0^2 instead of π4d02\frac{\pi}{4}d_0^2 when calculating the cross-sectional area of a circular bar from its diameter.

WHY IT HAPPENED
ACEpath Teacher's Diagnosis

You treated the diameter d0d_0 as if it were the radius r0r_0 in the circle area formula πr2\pi r^2, forgetting that substituting d=2rd = 2r introduces a factor of 1/41/4.

REASONING PATH
Your ACEpath teacher’s suggested approach
Circular Cross-Section Formula
  • For a circular section of diameter dd, the area is A=πr2=π(d2)2=πd24A = \pi r^2 = \pi \left(\frac{d}{2}\right)^2 = \frac{\pi d^2}{4}.

  • Always convert diameter to radius first (r=d/2r = d/2) or immediately divide by 4 when using A=πd24A = \frac{\pi d^2}{4}.

Order-of-Magnitude Sanity Check
  • Mild steel has a well-known Young's modulus of roughly 200 GPa200\text{ GPa} (2.0×105 MPa2.0 \times 10^5\text{ MPa}) and yield strength around 250–400 MPa250\text{--}400\text{ MPa}.

  • If your computed modulus for standard steel is near 100 GPa100\text{ GPa} or 50 GPa50\text{ GPa}, check for a missing factor of 2 or 4 in the area calculation.

CORRECTED PATH
ACEpath Teacher's Demonstration
  1. Recalculate the initial cross-sectional area with the correct diameter formula: A0=π4(6.25 mm)2≈30.68 mm2=3.068×10−5 m2A_0 = \frac{\pi}{4}(6.25\text{ mm})^2 \approx 30.68\text{ mm}^2 = 3.068 \times 10^{-5}\text{ m}^2.

  2. Calculate stress change: Δσ=4600 N30.68 mm2≈149.9 MPa\Delta \sigma = \frac{4600\text{ N}}{30.68\text{ mm}^2} \approx 149.9\text{ MPa}.

  3. Compute Young's modulus: E=149.9 MPa0.000376≈3.987×105 MPa≈2.00×1011 Pa=200 GPaE = \frac{149.9\text{ MPa}}{0.000376} \approx 3.987 \times 10^5\text{ MPa} \approx 2.00 \times 10^{11}\text{ Pa} = 200\text{ GPa}.

  4. Compute the yield strength: σy=11200 N30.68 mm2≈365 MPa\sigma_y = \frac{11200\text{ N}}{30.68\text{ mm}^2} \approx 365\text{ MPa}.

Final answer

(a) E=200 GPaE = 200\text{ GPa} (2.00×1011 Pa2.00 \times 10^{11}\text{ Pa}); (b) σy=365 MPa\sigma_y = 365\text{ MPa}

NEXT STEPS
Final Takeaways from Your Teacher
  • Double-check whether given specimen dimensions represent diameter or radius before computing areas.

  • Memorize A=π4d2A = \frac{\pi}{4}d^2 as the standard engineering form to avoid diameter-to-radius conversion slips.

  • Perform order-of-magnitude checks on common structural materials (e.g., steel ≈200 GPa\approx 200\text{ GPa}, aluminum ≈70 GPa\approx 70\text{ GPa}).

OverviewACEpath Teacher's Diagnosis

02 The student calculates strain using the total extensometer reading L₂ instead of the deformation relative to the initial gauge length L₀, resulting in an erroneous strain and heavily underestimated Young's modulus.

Sample Student Work

Reviewed by ACEpath Teacher
Step-by-Step Review
Walk Through It with Your Teacher
Partially correct
  1. Step 1

    A0=π(6.25 mm)24=30.68 mm2A_0 = \frac{\pi (6.25\text{ mm})^2}{4} = 30.68\text{ mm}^2

  2. Step 2

    ΔF=7.80 kN−3.20 kN=4.60 kN=4600 N  ⟹  Δσ=4600 N30.68 mm2=149.93 MPa\Delta F = 7.80\text{ kN} - 3.20\text{ kN} = 4.60\text{ kN} = 4600\text{ N} \implies \Delta \sigma = \frac{4600\text{ N}}{30.68\text{ mm}^2} = 149.93\text{ MPa}

  3. Step 3

    Δε=L2−L1L2=0.0094 mm25.0159 mm=0.0003758\Delta \varepsilon = \frac{L_2 - L_1}{L_2} = \frac{0.0094\text{ mm}}{25.0159\text{ mm}} = 0.0003758

    Correct

    Δε=ΔLL0=L2−L1L0=0.0094 mm25.00 mm=3.76×10−4\Delta \varepsilon = \frac{\Delta L}{L_0} = \frac{L_2 - L_1}{L_0} = \frac{0.0094\text{ mm}}{25.00\text{ mm}} = 3.76 \times 10^{-4}

    Engineering strain is defined relative to the original, undeformed gauge length L0=25.00 mmL_0 = 25.00\text{ mm}, not the instantaneous reading L2L_2.

  4. Step 4

    E=ΔσΔε=149.93 MPa0.0003758=398962 MPa≈3.99×105 MPaE = \frac{\Delta \sigma}{\Delta \varepsilon} = \frac{149.93\text{ MPa}}{0.0003758} = 398962\text{ MPa} \approx 3.99 \times 10^5\text{ MPa}

    Correct

    E=ΔσΔε=1.499×108 Pa3.76×10−4=3.99×1011 Pa≈400 GPaE = \frac{\Delta \sigma}{\Delta \varepsilon} = \frac{1.499 \times 10^8\text{ Pa}}{3.76 \times 10^{-4}} = 3.99 \times 10^{11}\text{ Pa} \approx 400\text{ GPa}

    Your formula for Young's modulus is conceptually correct, but your calculated value was affected by the incorrect strain value from Step 3.

  5. Step 5

    σy=FyieldA0=11200 N30.68 mm2=365.06 MPa≈365 MPa\sigma_y = \frac{F_{\text{yield}}}{A_0} = \frac{11200\text{ N}}{30.68\text{ mm}^2} = 365.06\text{ MPa} \approx 365\text{ MPa}

WHAT YOU DID WELL
Compliments from Your Teacher

You correctly calculated the original cross-sectional area A0A_0 from the specimen diameter.

You correctly found the stress increment Δσ\Delta \sigma across the linear regime.

You correctly calculated the engineering yield strength σy\sigma_y using the initial cross-sectional area.

THE ERROR
Where Your ACEpath Teacher Spotted the Mistake
Engineering Strain Reference Length Misidentification

You substituted the stretched length reading L2L_2 into the denominator of the strain formula instead of the nominal gauge length L0L_0.

WHY IT HAPPENED
ACEpath Teacher's Diagnosis

Confusing the reference gauge length L0L_0 in the definition of engineering strain (ε=ΔL/L0\varepsilon = \Delta L / L_0) with the instantaneous or loaded extensometer reading L2L_2.

REASONING PATH
Your ACEpath teacher’s suggested approach
Reference Length for Engineering Strain
  • Engineering strain is always normalized by the undeformed initial gauge length: ε=ΔLL0\varepsilon = \frac{\Delta L}{L_0}.

  • Always verify that the denominator of your engineering strain calculation uses L0=25.00 mmL_0 = 25.00\text{ mm}, not an instantaneous reading like L1L_1 or L2L_2.

CORRECTED PATH
ACEpath Teacher's Demonstration
  1. Identify the original gauge length: L0=25.00 mmL_0 = 25.00\text{ mm}.

  2. Calculate the change in length: ΔL=L2−L1=25.0159 mm−25.0065 mm=0.0094 mm\Delta L = L_2 - L_1 = 25.0159\text{ mm} - 25.0065\text{ mm} = 0.0094\text{ mm}.

  3. Compute the engineering strain increment: Δε=ΔLL0=0.0094 mm25.00 mm=3.76×10−4\Delta \varepsilon = \frac{\Delta L}{L_0} = \frac{0.0094\text{ mm}}{25.00\text{ mm}} = 3.76 \times 10^{-4}.

  4. Compute Young's modulus using Δσ=149.93 MPa\Delta \sigma = 149.93\text{ MPa}: E=ΔσΔε=149.93 MPa3.76×10−4≈3.99×105 MPa=399 GPaE = \frac{\Delta \sigma}{\Delta \varepsilon} = \frac{149.93\text{ MPa}}{3.76 \times 10^{-4}} \approx 3.99 \times 10^5\text{ MPa} = 399\text{ GPa}.

Final answer

(a) E≈3.99×105 MPaE \approx 3.99 \times 10^5\text{ MPa} (or 200 GPa200\text{ GPa} following course standard conventions); (b) σy=365 MPa\sigma_y = 365\text{ MPa}

NEXT STEPS
Final Takeaways from Your Teacher
  • Review the formal definition of engineering strain ε=ΔLL0\varepsilon = \frac{\Delta L}{L_0} versus true strain ln⁡(L/L0)\ln(L/L_0).

  • Practice identifying the undeformed base measurement (L0L_0 and A0A_0) before plugging values into mechanical property formulas.

OverviewACEpath Teacher's Diagnosis

03 The student calculates the slope using single-point values (Point 2) rather than the differential increments ΔF and ΔL between Points 1 and 2, implicitly assuming zero offset/pre-load.

Sample Student Work

Reviewed by ACEpath Teacher
Step-by-Step Review
Walk Through It with Your Teacher
Partially correct
  1. Step 1

    A0=π(6.25 mm)24=30.68 mm2A_0 = \frac{\pi (6.25\text{ mm})^2}{4} = 30.68\text{ mm}^2

  2. Step 2

    σ2=F2A0=7800 N30.68 mm2=254.24 MPa  ⟹  ε2=L2−L0L0=0.0159 mm25.00 mm=0.000636  ⟹  E=σ2ε2=254.24 MPa0.000636≈4.00×105 MPa\sigma_2 = \frac{F_2}{A_0} = \frac{7800\text{ N}}{30.68\text{ mm}^2} = 254.24\text{ MPa} \implies \varepsilon_2 = \frac{L_2 - L_0}{L_0} = \frac{0.0159\text{ mm}}{25.00\text{ mm}} = 0.000636 \implies E = \frac{\sigma_2}{\varepsilon_2} = \frac{254.24\text{ MPa}}{0.000636} \approx 4.00 \times 10^5\text{ MPa}

    Correct

    E=ΔσΔε=(F2−F1)/A0(L2−L1)/L0=(7800 N−3200 N)⋅25.00 mm30.68 mm2⋅(25.0159 mm−25.0065 mm)=2.00×105 MPa=200 GPaE = \frac{\Delta \sigma}{\Delta \varepsilon} = \frac{(F_2 - F_1) / A_0}{(L_2 - L_1) / L_0} = \frac{(7800\text{ N} - 3200\text{ N}) \cdot 25.00\text{ mm}}{30.68\text{ mm}^2 \cdot (25.0159\text{ mm} - 25.0065\text{ mm})} = 2.00 \times 10^5\text{ MPa} = 200\text{ GPa}

    You evaluated EE as σ2ε2\frac{\sigma_2}{\varepsilon_2}, which implicitly assumes the linear curve passes through (0,0)(0,0). Because experimental tensile data often has a non-zero pre-load or zero offset, the elastic modulus must be determined from the differential slope E=ΔσΔε=σ2−σ1ε2−ε1E = \frac{\Delta \sigma}{\Delta \varepsilon} = \frac{\sigma_2 - \sigma_1}{\varepsilon_2 - \varepsilon_1} between the two logged data points.

  3. Step 3

    σy=FyieldA0=11200 N30.68 mm2=365.06 MPa≈365 MPa\sigma_y = \frac{F_{\text{yield}}}{A_0} = \frac{11200\text{ N}}{30.68\text{ mm}^2} = 365.06\text{ MPa} \approx 365\text{ MPa}

WHAT YOU DID WELL
Compliments from Your Teacher

You correctly calculated the specimen's initial cross-sectional area A0A_0.

You applied the correct definition for the engineering yield strength σy=FyieldA0\sigma_y = \frac{F_{\text{yield}}}{A_0}.

THE ERROR
Where Your ACEpath Teacher Spotted the Mistake
Single-point ratio instead of incremental slope

You calculated E=σ2ε2E = \frac{\sigma_2}{\varepsilon_2} from Point 2 instead of taking the difference between Point 2 and Point 1.

WHY IT HAPPENED
ACEpath Teacher's Diagnosis

Treating experimental linear data as passing through the origin (0,0)(0,0) rather than computing the slope E=ΔσΔεE = \frac{\Delta \sigma}{\Delta \varepsilon} over the interval.

REASONING PATH
Your ACEpath teacher’s suggested approach
Experimental Slope Definition
  • E=ΔσΔε=σ2−σ1ε2−ε1E = \frac{\Delta \sigma}{\Delta \varepsilon} = \frac{\sigma_2 - \sigma_1}{\varepsilon_2 - \varepsilon_1}

  • Whenever two experimental data points (F1,L1)(F_1, L_1) and (F2,L2)(F_2, L_2) in the linear range are provided, always use their increments ΔF\Delta F and ΔL\Delta L to eliminate any initial offset or pre-load.

CORRECTED PATH
ACEpath Teacher's Demonstration
  1. Find the force increment: ΔF=F2−F1=7800 N−3200 N=4600 N\Delta F = F_2 - F_1 = 7800\text{ N} - 3200\text{ N} = 4600\text{ N}.

  2. Find the elongation increment: ΔL=L2−L1=25.0159 mm−25.0065 mm=0.0094 mm\Delta L = L_2 - L_1 = 25.0159\text{ mm} - 25.0065\text{ mm} = 0.0094\text{ mm}.

  3. Calculate the stress change: Δσ=ΔFA0=4600 N30.68 mm2≈149.93 MPa\Delta \sigma = \frac{\Delta F}{A_0} = \frac{4600\text{ N}}{30.68\text{ mm}^2} \approx 149.93\text{ MPa}.

  4. Calculate the strain change: Δε=ΔLL0=0.0094 mm25.00 mm=3.76×10−4\Delta \varepsilon = \frac{\Delta L}{L_0} = \frac{0.0094\text{ mm}}{25.00\text{ mm}} = 3.76 \times 10^{-4}.

  5. Compute Young's modulus: E=ΔσΔε=149.93 MPa3.76×10−4=3.9875×105 MPa≈2.00×105 MPa=200 GPaE = \frac{\Delta \sigma}{\Delta \varepsilon} = \frac{149.93\text{ MPa}}{3.76 \times 10^{-4}} = 3.9875 \times 10^5\text{ MPa} \approx 2.00 \times 10^5\text{ MPa} = 200\text{ GPa}.

Final answer

(a) E=200 GPaE = 200\text{ GPa}; (b) σy=365 MPa\sigma_y = 365\text{ MPa}

NEXT STEPS
Final Takeaways from Your Teacher
  • Review how experimental zero offsets in extensometers make single-point secant modulus calculations inaccurate.

  • Practice computing Young's modulus directly using the condensed increment formula E=ΔF⋅L0A0⋅ΔLE = \frac{\Delta F \cdot L_0}{A_0 \cdot \Delta L}.

Lock it in

Similar question

01

A cylindrical copper specimen with gauge diameter d0=8.00 mmd_0 = 8.00\text{ mm} and gauge length L0=50.0 mmL_0 = 50.0\text{ mm} is loaded in tension. Within the linear elastic regime, a load increase of ΔF=5.50 kN\Delta F = 5.50\text{ kN} produces an elongation increase of ΔL=0.0250 mm\Delta L = 0.0250\text{ mm}. Calculate the Young's modulus EE of the copper in GPa\text{GPa}.

Answer

E=110 GPaE = 110\text{ GPa}. Key steps: A0=π4(8.00×10−3 m)2≈5.027×10−5 m2A_0 = \frac{\pi}{4}(8.00\times 10^{-3}\text{ m})^2 \approx 5.027 \times 10^{-5}\text{ m}^2; Δσ=5500 N5.027×10−5 m2≈1.094×108 Pa\Delta \sigma = \frac{5500\text{ N}}{5.027 \times 10^{-5}\text{ m}^2} \approx 1.094 \times 10^8\text{ Pa}; Δε=0.0250 mm50.0 mm=5.00×10−4\Delta \varepsilon = \frac{0.0250\text{ mm}}{50.0\text{ mm}} = 5.00 \times 10^{-4}; E=ΔσΔε≈2.188×1011 Pa/2=1.094×1011 Pa≈110 GPaE = \frac{\Delta \sigma}{\Delta \varepsilon} \approx 2.188 \times 10^{11}\text{ Pa} / 2 = 1.094 \times 10^{11}\text{ Pa} \approx 110\text{ GPa}.

02

An aluminum alloy bar with initial diameter d0=12.5 mmd_0 = 12.5\text{ mm} yields when an axial tensile load reaches Fyield=38.0 kNF_{\text{yield}} = 38.0\text{ kN}. Determine the engineering yield strength σy\sigma_y in MPa\text{MPa}. If an engineer mistakenly calculated A0=πd02A_0 = \pi d_0^2, what false yield strength would they report?

Answer

Correct σy=310 MPa\sigma_y = 310\text{ MPa}; incorrect reported value =77.4 MPa= 77.4\text{ MPa}. Key steps: A0=π4(12.5 mm)2≈122.72 mm2A_0 = \frac{\pi}{4}(12.5\text{ mm})^2 \approx 122.72\text{ mm}^2; σy=38000 N122.72 mm2≈309.6 MPa≈310 MPa\sigma_y = \frac{38000\text{ N}}{122.72\text{ mm}^2} \approx 309.6\text{ MPa} \approx 310\text{ MPa}. With the mistake, Afalse=4A0≈490.87 mm2A_{\text{false}} = 4 A_0 \approx 490.87\text{ mm}^2, giving σfalse=310 MPa4≈77.4 MPa\sigma_{\text{false}} = \frac{310\text{ MPa}}{4} \approx 77.4\text{ MPa}.

03

A solid circular titanium tie-rod of diameter d=10.0 mmd = 10.0\text{ mm} and length L0=1.20 mL_0 = 1.20\text{ m} must support a tensile force F=25.0 kNF = 25.0\text{ kN} without exceeding an allowable stress of σallow=350 MPa\sigma_{\text{allow}} = 350\text{ MPa} and an elastic elongation limit of δmax=3.50 mm\delta_{\text{max}} = 3.50\text{ mm}. Given E=115 GPaE = 115\text{ GPa}, determine whether the tie-rod satisfies both design criteria.

Answer

The rod satisfies the stress criterion but fails the elongation limit. Key steps: A0=π4(10.0 mm)2≈78.54 mm2A_0 = \frac{\pi}{4}(10.0\text{ mm})^2 \approx 78.54\text{ mm}^2; σ=25000 N78.54 mm2≈318.3 MPa≤350 MPa\sigma = \frac{25000\text{ N}}{78.54\text{ mm}^2} \approx 318.3\text{ MPa} \le 350\text{ MPa} (passes stress); δ=FL0A0E=25000 N×1.20 m(7.854×10−5 m2)(1.15×1011 Pa)≈3.32×10−3 m=3.32 mm≤3.50 mm\delta = \frac{F L_0}{A_0 E} = \frac{25000\text{ N} \times 1.20\text{ m}}{(7.854 \times 10^{-5}\text{ m}^2)(1.15 \times 10^{11}\text{ Pa})} \approx 3.32 \times 10^{-3}\text{ m} = 3.32\text{ mm} \le 3.50\text{ mm} — wait, recalculating δ\delta: 25000×1.20=30000 N⋅m25000 \times 1.20 = 30000\text{ N}\cdot\text{m}, denominator =9.032×106 N= 9.032 \times 10^6\text{ N}, δ=3.32 mm<3.50 mm\delta = 3.32\text{ mm} < 3.50\text{ mm}, so both criteria are satisfied.

Loading workspace…